Quality
NDT for steel castings explained: UT, RT, MT and PT
Non-destructive testing proves a casting is sound without damaging it. Here is what each of the four common methods finds, and how to specify it.
· H.J. MetalCraft technical team

Every casting can contain discontinuities: shrinkage, gas porosity, inclusions or cracks. Non-destructive testing (NDT) finds them so you only receive sound parts. There are two groups: volumetric methods that look inside the metal, and surface methods that look for flaws at or just below the surface.
Volumetric methods
Radiographic testing (RT)
X-rays or gamma rays pass through the casting onto film or a detector. Denser metal blocks more radiation, so voids such as shrinkage and porosity show up as darker areas. RT gives a permanent record and is the classic method for pressure-retaining castings.
Ultrasonic testing (UT)
High-frequency sound is sent into the casting; reflections from internal flaws or the back wall are read on an instrument. UT is fast, portable, measures wall thickness, and suits thick sections where radiography is less sensitive.
Surface methods
Magnetic particle testing (MT)
The part is magnetised and dusted or sprayed with fine iron particles, which gather at surface and near-surface cracks that disturb the magnetic field. MT works only on ferromagnetic materials: carbon, alloy and martensitic stainless steels.
Dye penetrant testing (PT)
A coloured or fluorescent dye is drawn into surface-breaking flaws, excess is removed, and a developer draws the dye back out to reveal the flaw. PT works on any non-porous material, so it is the surface method for austenitic stainless, duplex and nickel alloys.
Which method when?
| Concern | Method |
|---|---|
| Internal shrinkage or porosity in a pressure boundary | RT or UT |
| Wall thickness, thick sections | UT |
| Surface cracks, carbon and alloy steel | MT |
| Surface cracks, stainless, duplex, nickel | PT |
How to specify NDT on your order
- Method: RT, UT, MT and/or PT.
- Extent: which areas (critical sections, weld preps, all surfaces) and what percentage of parts.
- Acceptance standard and level: the specification and severity level that defines a reject.
- Timing: after heat treatment, after rough machining, or after final machining.
Our NDT team
At H.J. MetalCraft, UT, RT, MT and PT are carried out under our NDT team of two Level II engineers and an ASNT-certified Level III. See quality control.
Have a casting in mind? Send us the drawing.
Request a quote