What is CF8M? Composition, properties and equivalents

CF8M is the cast equivalent of 316 stainless steel, made to ASTM A351, A743 and A744. This guide covers its chemistry, minimum properties, heat treatment, ferrite and equivalent grades.

· Husein Jazakallah, Managing Director

CF8M is the cast form of 316 stainless steel. It is an austenitic chromium-nickel-molybdenum grade, made to ASTM A351 for pressure-containing parts and to ASTM A743 and A744 for corrosion-resistant service. It is close to 316 but not identical: the cast chemistry is balanced differently and the metal normally contains some ferrite.

Is CF8M the same as 316?

No, but it is the nearest cast equivalent. Wrought 316 is made for rolling and forging, with roughly 16–18% chromium and 10–14% nickel. CF8M allows 18–21% chromium and 9–12% nickel, so the cast structure contains some ferrite in an austenite matrix. Both carry 2–3% molybdenum, and corrosion behaviour is broadly similar. A drawing that calls for CF8M should be quoted in CF8M, not 316.

What does the name CF8M mean?

CF8M is a designation from the Alloy Casting Institute (ACI) system, which ASTM uses for cast stainless grades.

  • C means the alloy is intended mainly for corrosion-resistant service. Heat-resistant grades start with H.
  • F identifies the nominal chromium-nickel type. ASTM describes CF8M as a 19% chromium, 10% nickel grade with molybdenum.
  • 8 is the maximum carbon in hundredths of a percent, so 0.08% carbon.
  • M shows that molybdenum has been added.

The same logic gives CF8 (no molybdenum) and CF3M (0.03% carbon maximum). The UNS number for CF8M is J92900.

What is the chemical composition of CF8M?

Composition limits per ASTM A351 for grade CF8M, in weight percent:

Element Limit (%)
Carbon (C) 0.08 max
Manganese (Mn) 1.50 max
Silicon (Si) 1.50 max
Phosphorus (P) 0.040 max
Sulphur (S) 0.040 max
Chromium (Cr) 18.0–21.0
Nickel (Ni) 9.0–12.0
Molybdenum (Mo) 2.0–3.0

Chromium gives the passive film. Nickel keeps the matrix mainly austenitic. Molybdenum improves resistance to pitting and crevice corrosion in chloride-bearing media, which is the main reason to choose CF8M over CF8.

What are the mechanical properties of CF8M?

Minimum room-temperature tensile requirements per ASTM A351 for CF8M:

Property Minimum
Tensile strength 485 MPa (70 ksi)
Yield strength (0.2% offset) 205 MPa (30 ksi)
Elongation in 50 mm (2 in) 30%

These are specification minimums in the solution-annealed condition. Actual results on a mill test certificate are usually higher. Austenitic grades such as CF8M cannot be hardened by heat treatment.

How is CF8M heat treated?

Per ASTM A351, CF8M is solution annealed. The castings are heated to at least 1040°C (1900°F), then quenched in water or cooled rapidly by other means. The standard notes that a higher temperature or a minimum holding time is sometimes needed.

Castings cool slowly in the mould. During that cooling, chromium carbides can form at grain boundaries and leave chromium-depleted zones that are open to intergranular attack. Solution annealing takes the carbides back into solution, and the fast quench stops them re-forming. It also restores ductility. Our heat treatment guide explains the process in more detail.

Why does ferrite matter in CF8M?

Because ferrite affects weldability, strength, toughness and corrosion. CF8M usually solidifies with a small amount of delta ferrite spread through the austenite. The amount depends mainly on the balance of ferrite-forming elements (chromium, molybdenum, silicon) against austenite-forming elements (nickel, carbon, manganese, nitrogen).

Some ferrite is useful. It reduces the risk of hot cracking during solidification and welding, and it raises strength. Too much ferrite has a cost. Long exposure at roughly 300–450°C embrittles the ferrite and lowers impact toughness, and the effect grows with ferrite content. Ferrite also makes the casting slightly magnetic.

ASTM A800 sets out how to estimate ferrite content from chemistry, by magnetic measurement or by metallography. If your application needs a ferrite range, state it on the order.

What are the equivalents of CF8M?

The closest European grade is EN 1.4408, GX5CrNiMo19-11-2, in EN 10213. It is near CF8M but not identical: EN 10213 sets carbon at 0.07% maximum, chromium at 18.0–20.0% and molybdenum at 2.0–2.5%. A casting made to one standard does not automatically meet the other, so check both if dual certification is needed.

Other designations you may meet:

  • ASME SA-351 CF8M, the ASME code version of A351
  • UNS J92900
  • JIS SCS14A, the Japanese grade aligned with CF8M

Where is CF8M used?

CF8M is used wherever 316-type corrosion resistance is needed in a cast shape. Typical parts include:

  • Pump casings and impellers
  • Valve bodies, bonnets and discs for butterfly, gate and ball valves
  • Strainer bodies and fittings
  • Process parts for chemical, offshore and water service

For help weighing CF8M against other alloys, see how to choose a casting material.

What is the difference between CF8M and CF3M?

Carbon. CF3M allows 0.03% carbon against 0.08% for CF8M. Its other limits are slightly wider (chromium 17.0–21.0%, nickel 9.0–13.0%), and the minimum tensile properties in ASTM A351 are the same. Lower carbon means less risk of carbide precipitation when the casting is welded and not re-annealed afterwards. Choose CF3M (EN 1.4409, the cast equivalent of 316L) for welded assemblies. CF8M is fine for parts that are solution annealed after any welding. Our comparison of CF8 vs CF8M vs CF3M sets the three grades side by side.

CF8M castings from H.J. MetalCraft

We cast CF8M to customer drawings in our Ahmedabad foundry. Sand castings run up to 180 kg per piece, and our investment casting unit makes parts from 10 g to 50 kg. Castings are solution annealed in-house and supplied raw or machined. See our stainless steel castings page, the standards and grades we cast to, and our investment casting capability, or send a drawing for a quote.

Equivalent grades are approximate. The grade and standard on your drawing govern.