Duplex vs super duplex castings: what is the difference?
Super duplex castings carry more chromium, molybdenum and nitrogen than standard duplex, which raises pitting resistance (PREN 40 and above) and strength. Here is how ASTM A890/A995 grades 4A, 5A and 6A compare.
· Husein Jazakallah, Managing Director
Super duplex has more chromium, molybdenum and nitrogen than standard duplex. That lifts its pitting resistance equivalent number (PREN) to 40 or more, against about 35 for a 2205-type duplex, and raises its minimum yield strength. In castings, standard duplex is usually ASTM A890/A995 grade 4A. Super duplex is usually grade 5A or 6A.
Both are austenitic-ferritic stainless steels, roughly half ferrite and half austenite. For the grades we pour, see duplex steel castings.
What is PREN and why does it matter?
PREN is a number that ranks resistance to pitting and crevice corrosion in chloride environments. It is calculated from the alloy's chemistry:
PREN = %Cr + 3.3 × %Mo + 16 × %N
For grades that contain tungsten, such as 6A, a modified form is often used: %Cr + 3.3 × (%Mo + 0.5 × %W) + 16 × %N.
Typical values:
- 2205-type duplex (cast grade 4A): about 35.
- Super duplex (cast grades 5A and 6A): 40 or higher. A PREN of 40 is the usual dividing line between duplex and super duplex.
PREN is a ranking tool, not a guarantee. The composition ranges are wide, so a heat at the bottom of every range has a lower PREN than one near the middle. If PREN matters, state a minimum on the order, calculated from the heat analysis.
Which cast grades are duplex and which are super duplex?
ASTM A890 covers duplex castings for general corrosion service. ASTM A995 covers duplex castings for pressure-containing parts such as valves, flanges and fittings. Both use the same grade numbers. The main ones are:
- 1B (CD4MCuN): a 25% chromium duplex with copper added. It is used for pumps handling abrasive, corrosive slurries.
- 4A (CD3MN): the 22% chromium standard duplex, the cast equivalent of 2205. The nearest European cast grade is EN 1.4470 (GX2CrNiMoN22-5-3).
- 5A (CE3MN): a 25% chromium super duplex, the cast equivalent of 2507. The nearest European cast grade is EN 1.4469 (GX2CrNiMoN26-7-4).
- 6A (CD3MWCuN): a 25% chromium super duplex with tungsten and copper added. It is usually described as the cast counterpart of wrought S32760.
The European grades are close but not identical, so check both standards before treating them as interchangeable.
How do 4A, 5A and 6A compare?
Composition in weight per cent, and minimum tensile properties, as given for ASTM A890/A995. All three grades have 0.03% carbon maximum.
| 4A (CD3MN) | 5A (CE3MN) | 6A (CD3MWCuN) | |
|---|---|---|---|
| UNS number | J92205 | J93404 | J93380 |
| Family | Duplex (2205 type) | Super duplex (2507 type) | Super duplex (W and Cu) |
| Chromium | 21.0–23.5 | 24.0–26.0 | 24.0–26.0 |
| Nickel | 4.5–6.5 | 6.0–8.0 | 6.5–8.5 |
| Molybdenum | 2.5–3.5 | 4.0–5.0 | 3.0–4.0 |
| Nitrogen | 0.10–0.30 | 0.10–0.30 | 0.20–0.30 |
| Other | Cu 1.0 max | — | Cu 0.5–1.0, W 0.5–1.0 |
| Tensile strength, min | 620 MPa | 690 MPa | 690 MPa |
| 0.2% yield strength, min | 415 MPa | 515 MPa | 450 MPa |
| Elongation, min | 25% | 18% | 25% |
Two points stand out. Grade 5A has the highest molybdenum and the highest minimum yield strength. Grade 6A has less molybdenum than 5A but adds tungsten and copper, and has a tighter nitrogen range. It gives up some yield strength in exchange for more ductility.
Always check the current edition of the standard and your own purchase specification. Project specifications for oil and gas often tighten these limits.
Why do solution annealing and quenching matter?
Duplex and super duplex castings must be solution annealed and then cooled quickly, normally by water quenching. Without it, they will not have the corrosion resistance or toughness the grade promises.
The reason is sigma phase and other intermetallic phases. These form when duplex steel spends time between roughly 700 °C and 950 °C. A thick casting cooling slowly in its sand mould passes through this range. Sigma is hard and brittle. It also takes chromium and molybdenum out of the surrounding metal, which leaves it less resistant to pitting.
Solution annealing heats the casting high enough to dissolve these phases. ASTM A890 and A995 set a minimum temperature for each grade. Rapid quenching then carries the casting through the danger range before sigma can form again. Super duplex grades, with more chromium and molybdenum, form sigma faster than standard duplex. That makes quench speed more critical for 5A and 6A, especially in heavy sections.
At H.J. MetalCraft we solution anneal duplex castings and quench them in an agitated 14,000-litre water tank. For more on furnace practice, see heat treatment of steel castings.
Note that ASTM A890 and A995 do not recommend these grades for service above 315 °C (600 °F), because embrittling phases can form at higher temperatures.
What ferrite content should you specify?
ASTM A890 and A995 do not set a ferrite limit. Both say the grades will develop approximately 30% to 60% ferrite, with the balance austenite.
Too much ferrite lowers toughness. Too little reduces strength and resistance to stress corrosion cracking. Many oil and gas specifications therefore set a narrower range. If yours does, put it on the order, with the measurement method, for example point count to ASTM E562 or a calibrated ferrite meter, because methods do not always agree.
For impact testing, corrosion testing to ASTM A923 or G48, and other supplementary checks, see NDT for steel castings and how to write a casting RFQ.
Where is each grade used?
Grade 4A is the general-purpose choice. It suits brackish water, chemical processing, pulp and paper and many oil and gas duties where chlorides are moderate. It is often chosen in place of 316-type castings when more strength or better resistance to stress corrosion cracking is needed.
Grades 5A and 6A are used where chloride levels or temperatures are higher. Typical parts are pump casings, impellers and valve bodies for seawater, produced water, firewater systems and desalination brine. Grade 6A is common in seawater and firewater systems on offshore installations.
How much more does super duplex cost?
Super duplex castings cost more than standard duplex. Grades 5A and 6A contain more nickel and molybdenum than 4A, and 6A adds tungsten and copper. Super duplex also needs tighter control of cooling and weld repair, and its orders more often carry ferrite, corrosion and impact tests.
The price gap moves with nickel and molybdenum prices, so we do not quote a fixed figure. Use 4A where its PREN is enough. Move to 5A or 6A when chloride level, temperature or a project specification calls for PREN 40 or above.
Getting a quote
We cast grades 4A, 5A and 6A as sand castings up to 180 kg per piece, with a minimum wall of 7 mm. See our capabilities for moulding, heat treatment and testing. We can supply castings raw or as machined components. For grade cross-references, see standards and grades. For austenitic grades, see stainless steel castings. For design limits and process choice, see steel casting tolerances and wall thickness and casting vs forging vs machining.