WCB vs WCC vs LCB vs LCC (and A105): what is the difference?

WCB and WCC are carbon steel castings for elevated-temperature service; LCB and LCC are impact-tested castings for low-temperature service; A105 is the forged equivalent. This note compares them side by side.

· Husein Jazakallah, Managing Director

WCB and WCC are carbon steel castings to ASTM A216 for ambient and high-temperature pressure service. WCC is the stronger of the two. LCB and LCC are castings to ASTM A352 that are Charpy impact tested at -46 °C, so they can be used at low temperatures. A105 is not a casting. It is the forged carbon steel commonly used alongside WCB.

How do the grades compare?

WCB WCC LCB LCC A105
Standard ASTM A216 ASTM A216 ASTM A352 ASTM A352 ASTM A105
Product form Casting Casting Casting Casting Forging
C, max % 0.30 0.25 0.30 0.25 0.35
Mn, max % 1.00 (up to 1.28 with reduced C) 1.20 (up to 1.40 with reduced C) 1.00 (up to 1.28 with reduced C) 1.20 (up to 1.40 with reduced C) 0.60 to 1.05 (up to 1.35 with reduced C)
Tensile strength 485–655 MPa (70–95 ksi) 485–655 MPa (70–95 ksi) 450–620 MPa (65–90 ksi) 485–655 MPa (70–95 ksi) 485 MPa (70 ksi) min
Yield strength, min 250 MPa (36 ksi) 275 MPa (40 ksi) 240 MPa (35 ksi) 275 MPa (40 ksi) 250 MPa (36 ksi)
Elongation, min 22% 22% 24% 22% 22% (round test bar)
Charpy impact test Not required by the base specification Not required by the base specification At -46 °C (-50 °F): 18 J (13 ft·lbf) average, 14 J (10 ft·lbf) single At -46 °C (-50 °F): 20 J (15 ft·lbf) average, 16 J (12 ft·lbf) single Not required by the base specification
Typical minimum service temperature -29 °C -29 °C -46 °C -46 °C -29 °C
Approximate EN equivalent GP240GH (1.0619), EN 10213 GP280GH (1.0625), EN 10213 G20Mn5 (1.6220), EN 10213 G20Mn5 (1.6220), EN 10213 Not a casting

The carbon and manganese rule is the same in A216 and A352. For each 0.01% of carbon below the maximum, manganese may rise by 0.04% above its maximum, up to the ceiling shown. A105 has its own rule: 0.06% more manganese for each 0.01% of carbon below the maximum. For A105 strip test specimens, the basic minimum elongation is 30%. The "average" Charpy value applies to the mean of three specimens.

What is the difference between WCB and WCC?

The difference is strength. WCC has a higher minimum yield strength, 275 MPa against 250 MPa for WCB. The tensile range is the same, 485 to 655 MPa, and so is the 22% minimum elongation.

WCC gets there with less carbon and more manganese. Its carbon limit is 0.25% against 0.30% for WCB, and its manganese limit is 1.20% against 1.00%. Lower carbon tends to help weldability.

In ASME B16.34, WCB is in material group 1.1 and WCC is in group 1.2, which carries higher pressure-temperature ratings. Designers choose WCC when they want a higher rating, or thinner walls for the same rating. Both grades come under the same graphitisation caution: B16.34 does not recommend prolonged use above about 425 °C.

For the full WCB data, see What is WCB material?

What is the difference between WCB and LCB?

The difference is low-temperature toughness. LCB is made to ASTM A352, the specification for castings for low-temperature service, and it requires a Charpy V-notch impact test at -46 °C. WCB has no impact requirement in its base specification, so it is usually limited to about -29 °C and above.

The chemistry limits for carbon and manganese are the same. LCB has a slightly lower tensile range (450 to 620 MPa) and yield (240 MPa), and a higher minimum elongation (24%).

Choose LCB, or LCC, when the minimum design metal temperature is below about -29 °C. That includes cold climates, depressurisation of gas lines, and refrigerated or chilled process lines. We give the same guidance on our carbon steel castings page.

What is the difference between LCB and LCC?

LCC is the stronger low-temperature grade, in the same way WCC is the stronger high-temperature grade. LCC has a minimum yield of 275 MPa against 240 MPa for LCB, and a tensile range of 485 to 655 MPa against 450 to 620 MPa.

The impact test temperature is the same, -46 °C. LCC has to meet higher energy values: 20 J average and 16 J single, against 18 J and 14 J for LCB.

A352 requires both grades to be normalised and tempered, or liquid quenched and tempered. LCC is often supplied quenched and tempered to reach both its strength and its toughness. In ASME B16.34, LCC is limited to 345 °C, well below the WCB and WCC limits. A low-temperature grade is not a substitute for WCB or WCC in hot service.

The usual EN cross-reference for both is G20Mn5 (1.6220) to EN 10213. Treat this one with care. EN 10213 tests G20Mn5 at a different impact temperature from A352, so check the toughness requirement directly rather than relying on the grade name.

Cast WCB or forged A105: when does a casting beat a forging?

A105 is a carbon steel forging specification for flanges, fittings, valves and similar piping parts. Its minimum tensile (485 MPa) and yield (250 MPa) match WCB. It has no upper tensile limit, but it caps hardness at 187 HB, and it allows more carbon, up to 0.35%.

A forging is usually the better choice for small, simple shapes such as flanges, small valve bodies and fittings. Forged parts start from wrought bar or billet, so internal porosity and shrinkage are less of a concern.

A casting tends to win when:

  • the part has internal passages, cavities or changing wall thickness that a forging would have to machine out
  • the part is too large or complex to forge economically in the quantities needed
  • near-net shape saves significant material and machining time
  • several features can be combined into one piece instead of being welded together

Casting quality has to be shown, not assumed. Radiography or ultrasonic testing of critical sections, plus magnetic particle testing of surfaces, gives the buyer evidence that the casting is sound. Our valve and pump castings page covers the parts we make most often.

Which grade should you specify?

Start from the design temperature and the pressure rating:

  • ambient to elevated temperature, standard rating: WCB
  • ambient to elevated temperature, higher rating: WCC
  • below about -29 °C down to -46 °C: LCB, or LCC where more strength is needed
  • small, simple shapes: consider A105 forgings

For alloy grades for higher temperatures or harsher media, see alloy steel castings. For our full cross-reference list, see standards and grades. Our PED material-manufacturer certificate covers sand castings; this note explains what that means for buyers. To check a grade against your part's size and section, send us your drawing.

Equivalents are approximate. The grade and standard on your drawing always govern.