What is WCB material? ASTM A216 WCB explained
WCB is the cast carbon steel grade of ASTM A216, used for valve bodies, flanges and fittings in pressure service. This note sets out its chemistry, properties, heat treatment and equivalents.
· Husein Jazakallah, Managing Director
WCB is a cast carbon steel made to ASTM A216, the specification for carbon steel castings suitable for fusion welding and high-temperature service. It is widely used for valve bodies, flanges and fittings in pressure service. The letters are commonly read as "weldable cast, grade B", though ASTM does not define them.
What does WCB stand for?
WCB is usually read as "weldable cast, grade B". This is the common reading, not an official one. ASTM A216 names three grades, WCA, WCB and WCC, but does not spell out the letters.
The "weldable" part does reflect the scope of the standard. A216 covers castings of a quality suitable for assembly with other castings or wrought steel parts by fusion welding.
What is ASTM A216?
ASTM A216 covers carbon steel castings for valves, flanges, fittings and other pressure-containing parts for high-temperature service. It has three grades. WCA is the lowest strength, WCB is the general-purpose grade, and WCC is the higher-strength grade. The standard says the choice depends on design, service conditions, mechanical properties and high-temperature characteristics.
For pressure equipment built to the ASME code, the matching material specification is SA-216 in ASME Section II.
What is the chemical composition of WCB?
ASTM A216 sets these maximum limits for WCB, in weight per cent. Phosphorus and sulphur are shown at the tighter limits given in datasheets for later editions:
| Element | WCB, max % |
|---|---|
| Carbon (C) | 0.30 |
| Manganese (Mn) | 1.00 |
| Phosphorus (P) | 0.035 |
| Sulphur (S) | 0.035 |
| Silicon (Si) | 0.60 |
| Copper (Cu), residual | 0.30 |
| Nickel (Ni), residual | 0.50 |
| Chromium (Cr), residual | 0.50 |
| Molybdenum (Mo), residual | 0.20 |
| Vanadium (V), residual | 0.03 |
| Total of residual elements | 1.00 |
The 2008 edition allowed up to 0.04% phosphorus and 0.045% sulphur. Certificates from older stock or older purchase specifications may still show those limits.
The carbon and manganese trade-off
A216 lets the foundry trade carbon for manganese. For each 0.01% reduction below the maximum carbon of 0.30%, manganese may rise by 0.04% above its 1.00% maximum. For WCB the ceiling is 1.28% manganese.
In practice this keeps strength up while carbon comes down. Lower carbon helps weldability and toughness, and manganese restores the tensile strength.
What are the mechanical properties of WCB?
ASTM A216 sets these room-temperature tensile requirements for WCB:
| Property | Requirement |
|---|---|
| Tensile strength | 485 to 655 MPa (70 to 95 ksi) |
| Yield strength, min | 250 MPa (36 ksi) |
| Elongation in 50 mm (2 in), min | 22% |
| Reduction of area, min | 35% |
Yield is measured by the 0.2% offset method or the 0.5% extension-under-load method. Tensile strength has an upper limit as well as a lower one. A casting that comes out too strong fails the specification just as one that is too weak does.
The base specification does not call for Charpy impact testing. Where low-temperature toughness matters, the usual answer is an impact-tested grade such as LCB or LCC to ASTM A352. See WCB vs WCC vs LCB vs LCC for the comparison.
How is WCB heat treated?
A216 requires castings to be supplied in the annealed, normalised, or normalised and tempered condition, unless the buyer orders Supplementary Requirement S15, quench and temper. Heat treatment is done after the castings have cooled below the transformation range, and furnace temperatures must be controlled by pyrometer.
Normalising is a common route for valve bodies. It refines the as-cast grain structure and gives more consistent tensile results through the section. For more on the options, see heat treatment of steel castings.
What is the temperature range for WCB?
WCB is commonly cited for service from -29 °C to 425 °C (-20 °F to 800 °F). The lower figure is the usual limit for carbon steel that has not been impact tested. The upper figure comes from ASME B16.34 practice. B16.34 notes that after prolonged exposure above about 425 °C the carbide phase of carbon steel may turn to graphite, and it does not recommend prolonged use above that temperature.
The actual pressure-temperature rating of a valve depends on its pressure class and the rating tables in B16.34, not on the material alone.
What is the EN equivalent of WCB?
The nearest European equivalent is GP240GH (material number 1.0619) to EN 10213. Both are weldable carbon steel castings for pressure service at elevated temperature. The two standards set different chemistry and property limits, so they are close but not interchangeable without checking.
Our standards and grades page lists other cross-references.
How does WCB compare with A105 and A106?
WCB is a casting. Its usual wrought counterparts are:
- ASTM A105, carbon steel forgings for piping components such as flanges, fittings and valve bodies.
- ASTM A106, seamless carbon steel pipe for high-temperature service, most often in Grade B.
WCB and A105 share the same minimum tensile strength (485 MPa) and minimum yield strength (250 MPa). That is why a WCB valve body and A105 flanges are often used together in the same line. A105 has no upper tensile limit, and its chemistry and test rules differ. The choice between a casting and a forging is covered in WCB vs WCC vs LCB vs LCC (and A105).
Where is WCB used?
Typical WCB parts include:
- gate, globe, check and ball valve bodies and bonnets
- pump casings and covers
- flanges, tees, elbows and other pressure fittings
- strainer bodies and compressor housings
It suits water, steam, oil, gas and other non-corrosive fluids at ambient and elevated temperatures. It is not a choice for corrosive media, where a stainless or alloy grade is needed, or for low-temperature service below about -29 °C.
What H.J. MetalCraft supplies in WCB
We cast WCB in our sand casting unit in Vatva, Ahmedabad, in pieces up to 180 kg. Our PED material-manufacturer certificate covers sand castings. See what PED certification means for casting buyers.
Each heat is checked by spectrometer. Tensile, hardness and NDT (UT, RT, MT and PT) testing can be added as the order requires. Castings are supplied raw or machined. Smaller parts from 10 g to 50 kg can be made by investment casting in our second unit.
For more on the grades we cast, see carbon steel castings, alloy steel castings and valve and pump castings. To price a part, send us your drawing.
Equivalents are approximate. The grade and standard on your drawing always govern.